Paperboard crease cracking should be investigated by separating damage in the printed finish from damage in the board, then checking material identity, crease geometry and the folding operation. Increasing pressure without identifying the failure can make the result worse. Start with retained flat blanks and compare them with samples after creasing and after folding. This guide explains how to build that comparison for folding cartons. It provides an inspection and supplier discussion plan, not a universal rule-and-matrix formula. Tooling dimensions and operating adjustments must come from the board supplier, die maker and instructions for the actual press.
Identify what has cracked
A white line on a dark printed fold does not describe the failure completely. Inspect a safely removed sample under consistent lighting and suitable magnification. Record whether the printed or coated layer alone has fractured, whether exposed fibres are visible, and whether the damage extends through the board. Keep a photograph of the unfolded blank beside the folded sample. An image of only the finished corner can conceal where the damage started.
Mark the affected fold on the drawing and identify its orientation within the sheet. Give each sample a material lot, sheet position and production checkpoint. If only one crease is affected, compare it with the other creases on the same blank. If every crease changes after a material delivery, compare the incoming board with a retained accepted lot before changing the whole die. These patterns select the next investigation; they do not independently prove a cause.
Distinguish cracking from an incorrect fold position. A carton can fold away from the intended line without showing the same surface rupture. It can also show both defects. Record the two results separately so that a tooling change cannot appear successful merely because one symptom became less visible. The downstream team should receive samples labelled with the actual observed defect, rather than a general instruction to “improve the crease.”
Understand the hinge before changing the tooling
Holmen’s creasing and folding explanation describes a crease as a prepared hinge in the board. A creasing rule presses the sheet into a matching channel, and the resulting fold should follow the intended bead direction. Its guidance also makes clear that board construction and tooling must be matched. These principles explain why copying one setup across unlike materials is unreliable; they do not authorize an arbitrary increase in pressure.
On a trial sheet, confirm which face receives the rule and which face carries the bead. Compare this with the approved fold drawing. Have the die maker review the rule profile, counter material and alignment if the hinge is poorly defined or visibly displaced. Record the actual tooling identification. A note saying “standard matrix” is insufficient when a replacement part may have a different geometry or condition.
The Realstar ML Series die-cutting and creasing machine supplies relevant equipment context for combined cutting and creasing. Confirm the supplied model and tooling arrangement before a trial. The product page is not a guarantee that any particular coated board will fold without cracking. A process acceptance sample remains necessary for the intended material, artwork and carton design.

Verify the board and its preparation
Record grade, supplier, lot, specified caliper and the sheet’s identified grain direction. Grammage alone is not enough to select a crease. Two stocks with similar mass per area can differ in construction and thickness. Ask the supplier for the current converting recommendations for the exact grade, including which measured property their tooling recommendation uses. Do not convert a nominal grammage into an assumed caliper and treat the result as a measurement.
Keep the storage and exposure history with the trial record. Note when a wrapped stack was opened, whether it moved between environments and how the material was protected between operations. Do not add water, steam or other improvised conditioning treatments to rescue a failing batch. If conditioning is suspected, agree the treatment and comparison method with the board supplier and retain untreated material for reference.
Check whether the artwork, varnish or laminate changed along with the board. Compare an unprinted trial where practical, but do not treat its success as acceptance of the finished printed structure. A fold through heavy coverage presents a different test sample from an unprinted white area. If the affected construction is laminated, use the complementary thermal lamination troubleshooting guide to separate finish defects from a poorly prepared hinge.
Map the failure to a production stage
Agree safe collection points before the trial. Keep a flat incoming blank, a creased but unfolded sample and a sample after the specified folding sequence. Where collection requires access to equipment, follow the installed machine’s isolation and access procedure. Never reach into the press or transport section to obtain a better diagnostic sample. If a checkpoint cannot be sampled safely, use a manufacturer-approved alternative.
Compare the same marked crease at each stage. Damage already present after printing belongs in the upstream record. Damage appearing immediately after creasing directs attention to the board-tooling interaction. A crease that looks intact before folding but splits afterwards needs a review of fold orientation, forming sequence and material performance. This stage comparison is more informative than repeatedly inspecting only the final stacked carton.
| Observation | Record to keep | Next controlled comparison | Conclusion to avoid |
|---|---|---|---|
| Only the printed finish shows a line | Artwork version and magnified fold image | Approved finish construction on comparable creases | Every visible line means the board split through |
| One crease differs across the sheet | Sheet position and tooling reference | Affected location against an accepted location | The whole material lot is defective |
| Cracking begins only after folding | Before-fold and after-fold samples | Approved fold direction and sequence | More press pressure must solve it |
| New lot differs from retained stock | Grade, caliper, lot and exposure history | Matched trials with the approved tooling | Equal grammage means identical converting behaviour |
| Fold position wanders without rupture | Drawing reference and fold location | Crease definition and downstream guidance | Misfolding and cracking are the same defect |
This table organizes observations rather than supplying machine settings. Use the board supplier’s grade-specific instructions and the die maker’s approved tooling data to choose each trial condition. Keep successful and unsuccessful samples together until the cause has been reviewed.
Review tooling condition and local consistency
Ask qualified personnel to compare the installed rule and channel with the approved specification. Check identification, visible damage, wear and the condition of the supporting surfaces through the authorized inspection procedure. Record any repair or replacement before producing another trial. A setup described as unchanged may still differ if a worn component was exchanged or a counter was fitted in a different location.
If the defect repeats in a particular sheet area, preserve a position map. Compare the intended crease with nearby cuts and folds, including whether the sheet remains correctly located during the operation. The relationship matters when cutting and creasing share a press cycle. Use the die cutting, stripping and blanking guide to keep these process functions distinct in the investigation record.
For jobs transferred to another press, confirm compatibility rather than assuming the old recipe travels unchanged. The accompanying CNC die-cutting photograph shows a separate Realstar configuration, not a replacement component for the ML Series. A transferred job needs its own approved tooling and acceptance check. Differences in machine arrangement should be discussed with the supplier before using old control values as trial instructions.
Run a trial that can answer one question
Write the trial question before running sheets. For example, determine whether the approved tooling arrangement produces different results on a suspect lot and a retained lot under comparable preparation. Keep the artwork, fold direction, inspection method and relevant setup constant. If multiple conditions must change, label the result as a combined process trial instead of attributing improvement to one variable.
Define acceptance before selecting the best-looking sample. Specify which faces are visible in use, the viewing conditions, the required fold position and any repeated opening requirement. Include the customer’s functional requirements as well as appearance. A neatly folded carton that fails during erection has not passed simply because its outer surface looks good at machine exit. Avoid inventing a universal permitted crack length or visual grade.
Include the normal production sequence in the confirmation run. Check startup samples, samples from the agreed stable run and samples after the next relevant finishing step. Record when each was collected. If inspection depends on a waiting period supplied by a coating or adhesive manufacturer, identify that period and its source in the job record. Do not silently compare freshly finished samples with older reference cartons.

Keep collection and troubleshooting safe
HSE’s printing machinery safety overview supports the need for suitable safeguarding and controlled intervention around presses and finishing machinery. Apply the site’s risk assessment and the actual machine documentation. A stationary photograph in this article does not show that a machine is isolated, safe to reach into or authorized for a particular intervention.
The following WorkSafeBC education explains guarding and lockout responsibilities in manufacturing. It provides safety context for tooling inspection and sample collection, rather than instructions for setting a creasing press. Machine-specific servicing must remain with appropriately trained personnel using the supplied procedures.
Watch WorkSafeBC guards and lockout training on YouTube.
Prepare the supplier review and purchasing brief
Send the board and tooling identities, marked drawings, checkpoint samples and trial results together. Ask the board supplier which grade-specific converting recommendations apply and ask the die maker how the installed geometry compares with the intended fold. Include the intended finishing sequence. A request containing only a photograph of a cracked carton usually leaves too many uncontrolled possibilities for a reliable recommendation.
For equipment discussions, describe the actual board range, artwork, carton styles, batch pattern and acceptance samples. Review the relevant Realstar machinery range and keep upstream crease quality separate from downstream handling capacity. The folder gluer collector capacity guide addresses output handling; a collector should not be expected to repair a damaged hinge. Retain the approved trial as the reference for future material or tooling changes.
Frequently asked questions
Should more pressure fix paperboard crease cracking?
Not automatically. Identify the damaged layer and the stage where the defect first appears, then compare the board and tooling with the approved specification. Pressure changes require machine-specific authorization and a controlled trial; a visible crack alone does not establish the correct adjustment.
Can two boards with the same grammage use identical crease tooling?
Not by assumption. Confirm actual grade, caliper, construction and grain orientation, then obtain the material supplier’s recommendation. Equal grammage does not independently establish matching thickness or folding behaviour.
Is an unprinted folding sample sufficient for acceptance?
It is useful for comparison, but the final printed, coated or laminated construction still needs the agreed folding and appearance checks. Record both samples so that a finish-related difference remains visible.